湖北农业科学 ›› 2025, Vol. 64 ›› Issue (8): 97-103.doi: 10.14088/j.cnki.issn0439-8114.2025.08.015

• 资源·环境 • 上一篇    下一篇

平菇菌渣生物炭的制备及对水中铅、镉离子的吸附效果

陈花1,2, 常宇航1, 张佳怡1, 李强1,2   

  1. 1.榆林学院生命科学学院,陕西 榆林 719000;
    2.陕西省陕北矿区生态修复重点实验室,陕西 榆林 719000
  • 收稿日期:2025-03-04 出版日期:2025-08-25 发布日期:2025-09-12
  • 作者简介:陈 花(1979-),女,山西神池人,副教授,硕士,主要从事固废循环农业等方面的研究,(电子信箱)510697622@qq.com。
  • 基金资助:
    陕西省教育厅2022年度重点科研计划项目(重点实验室项目)(22JS046); 2022年榆林市科技局产学研项目(CXY-2022-62)

Preparation of biochar from spent Pleurotus ostreatus substrate and its adsorption effect on lead and cadmium ions in water

CHEN Hua1,2, CHANG Yu-hang1, ZHANG Jia-yi1, LI Qiang1,2   

  1. 1. College of Life Sciences, Yulin University, Yulin 719000, Shaanxi, China;
    2. Shaanxi Key Laboratory of Ecological Restoration in Northern Shaanxi Mining Area, Yulin 719000, Shaanxi, China
  • Received:2025-03-04 Published:2025-08-25 Online:2025-09-12

摘要: 为缓解农业固体废弃物堆积引发的环境污染,以平菇菌渣为材料,采用不同热解温度(300~800 ℃)制备生物炭,并通过SEM-EDS、BET和FTIR等技术对所制备的生物炭进行表征分析。结果表明,随着热解温度升高,生物炭的pH先升高后降低,产率降低,C含量上升而O含量下降,芳香性增强。300~750 ℃时,随着热解温度的升高,孔隙数量逐渐增加且排列趋于均匀;800 ℃时,孔状结构坍塌,比表面积和孔容减小。高温下官能团振动强度减弱,750 ℃制备的生物炭中CaCO3含量增加,有助于吸附重金属离子。750 ℃制备的生物炭处理重金属超标污水的结果表明,生物炭投加量为4 g/L时,对Pb2+和Cd2+的吸附率分别达97.63%和92.01%,表现出优异的吸附性能。

关键词: 平菇菌渣, 生物炭, 热解温度, 重金属, 铅, 镉, 水体, 吸附

Abstract: To alleviate environmental pollution caused by the accumulation of agricultural solid waste, spent Pleurotus ostreatus substrate was used as raw material to prepare biochar at pyrolysis temperatures ranging from 300 to 800 ℃. The biochars were characterized using SEM-EDS, BET, and FTIR techniques. The results showed that as the pyrolysis temperature increased, the pH of the biochar initially rose and then declined, the output capacity decreased, the carbon content increased while the oxygen content decreased, and aromaticity was enhanced. When the pyrolysis temperature ranged from 300 to 750 ℃, the number of pores gradually increased and their arrangement became uniform as the pyrolysis temperature rose; however, at 800 ℃, the porous structure collapsed, resulting in reduced specific surface area and pore volume. The intensity of functional group vibrations weakened at higher temperatures, and the CaCO3 content in biochar produced at 750 ℃ increased, promoting the precipitation of heavy metal ions. The results of heavy metal wastewater treatment by biochar prepared at 750 ℃ showed that the adsorption rate of Pb2+ and Cd2+ reached 97.63% and 92.01%, respectively, when the biochar dosage was 4 g/L, showing excellent adsorption performance.

Key words: spent Pleurotus ostreatus substrate, biochar, pyrolysis temperature, heavy metal, lead, cadmium, water body, adsorption